Twenty defects, their standardised number, where in the joint they form and what they look like on a radiographic film.


An inspection report announcing "linear indication at joint 14" means little to anyone who has not spent years at a film viewer. This page closes that gap: it describes the defects actually encountered on shop and site welds, with the standardised vocabulary that lets people discuss them without ambiguity.

Every defect carries a number defined by EN ISO 6520-1. That number is not inspector's affectation: it is what makes a Belgian, German or Spanish report read the same way. When you see 401, it is a lack of fusion, whatever language the document is in.

Reading a film: more metal, lighter image

Everything else follows from that single principle. The radiation passes through the part and exposes the film. Where there is less material — a pore, a crack, missing metal — more radiation gets through and the film is darker. Where there is more material, or more absorbent material, it is lighter.

That explains almost every image below. A pore is a void: dark spot. Lack of penetration is a continuous void at the root: dark band. Excess penetration is metal to spare: light area.

And it explains the exception that catches everyone out: a tungsten inclusion appears lighter than its surroundings. Tungsten absorbs radiation far more than steel does. It is the only common defect that reads the other way round, and it is also why you spot it instantly once you know what to look for.

Three families, and why that decides the method

Sorting defects into families is not an academic exercise: it determines which method stands a chance of finding them.

Planar defects — cracks, lack of fusion, lack of penetration. Two dimensions and almost no thickness. Radiography sees them only if the beam catches them on the right axis; badly oriented, they can pass unnoticed. Ultrasonics is good on them: a flat surface reflects. They are also the most serious defects, because they concentrate stress.

Volumetric defects — porosity, slag inclusions, cavities. They have volume, so radiography renders them very well, with a telling image. Ultrasonics detects them but characterises them less finely.

Geometric defects — misalignment, undercut, concavity, excess penetration. These affect the shape of the joint rather than its internal health. Many are visible to the eye, which is why visual testing to EN ISO 17637 remains the foundation of everything: it is carried out on all welds, whatever the execution class.

What is never acceptable

Three fixed points from EN ISO 5817. They are worth knowing because they settle arguments.

Cracks are not permitted at any quality level. Not B, not C, not D. A crack is repaired, not negotiated. Only microcracks and crater cracks fall under separate rules.

Lack of fusion is permitted at neither B nor C. At level D a distinction applies: surface-breaking, it remains prohibited; internal, it may be tolerated if it stays a short imperfection, within the limits the standard sets. That nuance is flattened by most summaries, and it has consequences at handover.

Incomplete root penetration is permitted at neither B nor C, and is permitted at level D within limits — for butt joints, only on full penetration welds made from one side.

We do not publish the numerical limits: they are in the standard, they depend on thickness and joint type, and a figure copied out of context is a trap. What is above is enough to know whether you have a serious problem or a point to discuss.

Twenty defects in radiographic images

The films below come from our interpretation documentation. For each: where the defect forms in the joint, its standardised number, and what it produces on the image. The arrows and markers on the films are part of the original documents.

Sidewall lack of fusion

ISO 6520-1 — 401 / 4011

Radiographic film showing sidewall lack of fusion in a weld

Where it forms: At the interface between weld metal and the bevel face: the pool did not bond the parent metal.

On the film: Straight lines of darker density, narrow, parallel to the bead or isolated, running lengthwise. Sometimes dotted with blacker points.

The detail that counts: these lines are straight. A slag inclusion gives sinuous lines. That is often what settles the question between the two on a film.

Inter-run lack of fusion

ISO 6520-1 — 401 / 4012

Radiographic film showing lack of fusion between two weld runs

Where it forms: Between two successive runs, along the surface of the bead already deposited. Usual cause: insufficient heat input.

On the film: Small darker points, some drawn out into a fine tail aligned with the direction of welding. They sit not at the centre of the bead but towards its edges.

The off-centre position is the clue: what appears at the centre belongs to the root.

Incomplete root penetration

ISO 6520-1 — 4021

Radiographic film showing incomplete root penetration in a weld

Where it forms: At the bottom of the preparation: the root faces were not fused together. Typical of a single-V preparation, with or without a root face.

On the film: Long band of darker density, continuous and narrow, at the centre of the bead, with sharp edges.

Not permitted at levels B and C. Permitted at level D within the limits of the standard, and only on full penetration welds made from one side.

Longitudinal crack

ISO 6520-1 — 100

Radiographic film showing a longitudinal crack in the weld metal

Where it forms: In the deposited metal, running along the length of the weld.

On the film: Irregular dark line, spiral or feather-shaped, following the centre of the bead.

Never permitted, at any quality level.

Transverse crack

ISO 6520-1 — 100

Radiographic film showing a transverse crack across the weld

Where it forms: In the deposited metal, perpendicular to the axis of the weld.

On the film: Irregular dark line crossing the width of the weld zone.

Often associated with hydrogen and restraint. It can appear hours after welding — hence the waiting periods before testing.

Longitudinal root crack

ISO 6520-1 — 100

Radiographic film showing a longitudinal crack at the root of the joint

Where it forms: In the deposited metal, along the root of the joint.

On the film: Dark lines following the root.

Do not confuse with lack of penetration. A crack is characterised by "broken", irregular lines; lack of penetration gives a continuous band with sharp edges. It is the most common confusion on a film, and the two are not repaired the same way.

Scattered porosity

ISO 6520-1 — 2011 / 2012

Radiographic film showing scattered porosity in the bead

Where it forms: Gas pockets trapped in the weld metal on solidification, randomly distributed.

On the film: Small round darker spots, of varying size, scattered through the weld zone.

Often linked to moisture, poorly baked electrode coating or failing gas shielding.

Clustered porosity

ISO 6520-1 — 2013

Radiographic film showing a cluster of agglomerated porosity

Where it forms: The same gas pockets, but grouped into a localised cluster rather than distributed.

On the film: Round or slightly elongated spots, grouped together in one or more places.

A cluster is treated differently from scattered porosity: the standard looks at it as a whole, because a cluster can also mask another defect behind it.

Linear porosity at the root

ISO 6520-1 — 2014

Radiographic film showing porosity aligned along the root

Where it forms: Along the joint, on the axis of the root.

On the film: Round or elongated spots aligned in a straight line at the centre of the weld zone.

Alignment at the centre points to the root run and its gas shielding.

Inter-run slag inclusions

ISO 6520-1 — 300 / 301

Radiographic film showing slag inclusions between weld runs

Where it forms: Non-metallic impurities solidified on the surface of a run and poorly removed before the next.

On the film: Irregular shapes of darker density, narrowly elongated, randomly placed across the image.

Primarily an execution fault: it is prevented by proper de-slagging between runs.

Slag inclusions in parallel lines (wagon tracks)

ISO 6520-1 — 300 / 301

Radiographic film showing slag inclusions in parallel lines, known as wagon tracks

Where it forms: Same origin, but the slag stays trapped along the edges of a run over a long length.

On the film: Parallel dark lines running lengthwise — hence the name.

These lines are sinuous, unlike the straight lines of lack of fusion. That is the distinguishing criterion on a film.

Tungsten inclusions

ISO 6520-1 — 304

Radiographic film showing tungsten inclusions appearing light

Where it forms: TIG welding: a fragment of the refractory tungsten electrode has fallen into the weld pool.

On the film: Irregular shapes LIGHTER than their surroundings, randomly placed.

The only common defect that appears light. Tungsten absorbs radiation far more than steel: less radiation reaches the film, so the image there is paler.

External undercut

ISO 6520-1 — 5011 / 5012

Radiographic film showing external undercut at the weld toe

Where it forms: On the outer surface, at the weld toe: the arc has thinned the parent metal and it has not been filled.

On the film: Irregular zone of darker density along the edge of the bead.

The density of undercut is always darker than that of the parent parts — that is what distinguishes it from a simple edge effect.

Root-side undercut (shrinkage groove)

ISO 6520-1 — 5013

Radiographic film showing undercut on the root side

Where it forms: On the inner surface, along the root: the parent metal is thinned at the edge of the root run.

On the film: Irregular zone of darker density, not far from the centre, running along the edge of the root run.

On pipework this is the defect you will never see by eye: the surface concerned is inside the pipe.

Excessive cap concavity (incompletely filled groove)

ISO 6520-1 — 511

Radiographic film showing excessive concavity of the capping run

Where it forms: At the capping run: the amount of filler is insufficient and the top of the bead is hollow.

On the film: Darker density extending across the full width of the weld zone; the rest of the part looks lighter.

Direct consequence: the effective thickness of the joint is reduced there. It is a section defect, not merely a cosmetic one.

Root concavity

ISO 6520-1 — 515

Radiographic film showing concavity at the root of the joint

Where it forms: On the inner surface, a depression at the centre of the bead at the root.

On the film: Elongated irregular area, darker, with fuzzy edges, at the centre of the bead width.

The fuzzy edges distinguish it from lack of penetration, whose edges are sharp.

Localised root crater

ISO 6520-1 — 515

Radiographic film showing a localised crater at the root

Where it forms: The same phenomenon as root concavity, but severe and confined to a short distance.

On the film: Localised, distinctly darker area over a short length, with a fuzzy edge. It can be wider than the root run itself.

Often linked to an arc restart or a badly executed stop.

Excessive penetration (icicle)

ISO 6520-1 — 504

Radiographic film showing excessive penetration at the root

Where it forms: At the root: too much filler has passed through and hangs inside the joint.

On the film: LIGHTER density at the centre of the weld zone. It may run the whole length or affect isolated areas only.

On pipework in service an icicle is not just a cosmetic defect: it disturbs the flow and can initiate localised corrosion.

Linear misalignment (Hi-Lo)

ISO 6520-1 — 507 / 5071

Radiographic film showing misalignment of the parts to be welded

Where it forms: The two parts to be joined are not in the same plane: a step in thickness at the joint.

On the film: Abrupt change in density across the full width of the bead image, running lengthwise.

A fit-up fault, not a welding fault. It is corrected at assembly and is very expensive to put right afterwards.

Misalignment with insufficient root fill

ISO 6520-1 — 507 + 511

Radiographic film showing misalignment combined with insufficient root filling

Where it forms: The two defects compound: parts offset and root insufficiently filled.

On the film: Abrupt change in density at the centre of the bead width, with a darker area running lengthwise.

The combination is common: a badly aligned joint fills badly. It is also why fit-up matters as much as welding.

Standards cited in this article

  • EN ISO 6520-1:2007 — Classification of geometric imperfections in metallic materials — Part 1: fusion welding
  • EN ISO 5817:2023 — Quality levels for imperfections in fusion-welded joints in steel, nickel, titanium and their alloys
  • EN ISO 17635:2025 — Non-destructive testing of welds — General rules for metallic materials
  • EN ISO 17636-1 — Radiographic testing of welds — Part 1: X- and gamma-ray techniques with film
  • EN ISO 17637 — Visual testing of fusion-welded joints
  • EN ISO 10675-1:2021 — Acceptance levels for radiographic testing — Part 1: steel, nickel, titanium and their alloys

The editions given are those verified with the issuing body at the time of writing. Standards are copyright works: we reproduce neither their text nor their tables. They are available from NBN or from your national standards body.

This article is an explanation, not a specification. It does not replace the standard in any way, and it deliberately contains no limit values and no numerical acceptance criteria. Where they differ, the applicable edition of the standard and your project specification prevail. For a specific case, call us.

Need a reliable inspection for your installations?

Our certified technicians respond promptly across all of Belgium. Contact us today for a customised quote and ensure the compliance of your equipment.